Tuesday, April 14, 2020

Sop Concrete Block free essay sample

Standard Operating Procedures of Making a Concrete Block. | Department/ Unit: | This Standard Operating Procedures has been done by Department of Production and Manufacturing of Concrete Block| Purpose:| The purpose of this Standard Operating Procedures of making a concrete block is to provide instructions in order to manufacture a concrete block. | Who can perform this SOP:| Skilled worker technician. | Equipment/ Tools Needed:| Personal Protective Equipment:| Safety helmet, goggles, hand gloves and face mask. Tools:| Sand, cement, water, gravel and formwork. | Reference Materials:| http://www. madehow. com/Volume-3/Concrete-Block. html | Others: | None| Ref No| 1993/123| Date| 16 April 2013| Page No. | 2| Procedures: | Mixing Process 1. Store the sand and gravel outside in piles. 2. Transfer them into storagebins by conveyer belts. 3. Store the portland cementInto large vertical silos to avoidmoisture. 4. Transfer the required amount of sand. gravel and cement by mechanicalmeans to a weigh batcher to measurethe amount of each material. 5. Flow the weighed materials into a stationary mixer and blend themtogether for several minutes. We will write a custom essay sample on Sop Concrete Block or any similar topic specifically for you Do Not WasteYour Time HIRE WRITER Only 13.90 / page 6. Add small amount of water to the mixer. | Molding 1. Dump the thoroughly mixed concreteto an inclined bucket conveyer and transport it to an elevated hopper. 2. Convey the concrete to another hopper on top of the block machine at a measured flow rate . When they are full so that the downward force will mold the concrete. The upper mold head will compact the molds 3. Push the compacted molds down and out of the molds onto a flat steel pallet. . Push the pallet and blocks out of the machine onto a chain conveyer. | Curing 1. Convey the pallets of blocks to an automated stacker that will place them in a curing rack. Move the rack into a curing kiln when it is full. 2. Hold the blocks in the kiln for 1 to 3 hours. 3. Introduce steam gradually into the kiln to raise the temperature not more than 16? C per hour. 4. Cure the blocks at a temperature of (66-74? C) 5. Upon reaching the curing temperature shut the steam off. 6. Soak the blocks in hot moist air for 12-18 hours. 7. Dry the blocks after soaking in the kiln again by further raising the temperature for 3 hours. | Cubing 1. Roll the racks of cured blocks out of the kiln. 2. Unstack the pallets of blocks and place them on a chain conveyer. 3. Push the blocks off from steel pallets and fed the empty pallets back into block machine. 4. Pass the blocks through a cuber which aligns aligns each block and stack them into cube three blocks across by six blocks deep by three or four blocks high. 5. Carry the blocks outside with a forklift. Place them in a storage. | Prepared by: | Skilled worker technician. Reviewed by: | Project Manager from Production and Manufacturing of Concrete Block. | Approved by: | Chief Manager from Quality Department of Production and Manufacturing of Concrete Block. | Ref No| 1993/123| Date| 16 April 2013| Page No. | 3| Standard Operating Procedures of Making a Concrete Block UHL2422 English for Technical Communication NAME| STUDENT ID| Mohd Adhan Izmi Bin Roslan| AA12227| Wan Mo hd Haziq Bin Wan Mohd Kamil| AA12080| Maxwell Sayong| TB12022| Jason Osen Anak Ahok| PA12021| LECTURER| Mdm. Aisyah Hanum Binti Abu Bakar|

No comments:

Post a Comment

Note: Only a member of this blog may post a comment.